Materials Today Communications 43 (2025) 111749 Contents lists available at ScienceDirect Materials Today Communications journal homepage: www.elsevier.com/locate/mtcomm Hole expansion performance and microstructure evolution of QP steel: Influence of low-frequency vibration amplitude Qi Li a , Wen Zhang a , Xincun Zhuang a,b,* , Huachao Yang a , Han Sun a, Zhen Zhao a,b,* a Institute of Forming Technology and Equipment, School of Materials Science and Engineering, Shanghai Jiao Tong University, Shanghai 200030, China National Engineering Research Center of Die & Mold CAD and State Key Laboratory of Metal Matrix Composites, Shanghai Jiao Tong University, Shanghai 200030, China b A R T I C L E I N F O A B S T R A C T Keywords: Vibration-assisted forming Hole expansion QP steel Dislocation TRIP effect Vibration-assisted forming is a novel forming process that has beneficial effects such as improving forming limit compared to conventional forming process. In this study, an electro-hydraulic excitation device was used to conduct low-frequency vibration assisted hole expansion (LFVHE) tests with QP steel. To explain the effect of low-frequency vibration on the hole expansion performance, the microstructure evolution of QP steel was investigated by electron backscatter diffraction (EBSD), transmission electron microscope (TEM) and nano­ indentation. In addition, various fabrication methods including wire cutting and laser cutting were adopted for the inner hole of QP steel. The results indicate that compared to conventional hole expansion, the hole expansion ratio (HER) is improved after the superposition of vibration with an amplitude of 0.062 mm, while HER de­ creases with the increasing amplitude in the vibration frequency of 30 Hz. The proliferation of dislocations within the ferrite grains increases the hardness of ferrite with an amplitude of 0.062 mm. And significant annihilation of dislocations decreases the hardness of ferrite when the amplitude increases to 0.243 mm. A low hardness difference between ferrite and martensite is conducive to improving HER. In addition, the proliferation of dislocations after superimposing low-frequency vibration promotes the transformation induced plasticity (TRIP) effect of QP steel, and there is a positive correlation with amplitude. 1. Introduction Advanced high-strength steel (AHSS) has attracted increasing attention owing to its light weighting opportunities in automotive ap­ plications [1] leading to improving fuel economy and reducing emis­ sions. To date, AHSSs have developed up to the third generation [2], among which the representative ones are dual phase (DP) steel [3], quenched and partitioned (QP) steel [4], and martensitic steel [5]. The martensitic structure of DP, QP, and martensitic steels ensures high tensile strength exceeding 1000 MPa, which is a significant improve­ ment over traditional low-carbon steels [6]. Currently, AHSS is widely stamped into automotive safety parts [7] such as B-pillars, door rein­ forcing beams and bumper beams. However, the limited formability and high crack sensitivity of AHSS make it prone to cracking during the stamping process [8]. The formability of AHSS is widely evaluated by the hole expansion test [9] for its ability to effectively investigate its resistance to sheet metal cracking. Hole expansion performance of AHSS is influenced by the original microstructure of the material and the fabrication method. The original microstructure of AHSS includes phase morphology, hardness difference between ferrite and martensite, and second-phase particles. Terrazas et al. [10] used DP980 to study the hole-expansion performance of different martensite morphologies and concluded that martensite with a fine and uniform distribution favours HER enhance­ ment. Chen et al. [11] demonstrated that a large hardness difference between ferrite and martensite causes cracks at the interface, which lowers the overall HER. Xu et al. [12] studied the effect of second-phase particles of TWIP steel on HER. The detachment of second-phase parti­ cles from the matrix resulted in a decrease in shear resistance. In addi­ tion, the hole expansion performance of AHSS can also be affected by the fabrication method of inner hole. Hance et al. [13] discovered that the HER of dual phase steel and austenitic stainless steel in the pierced-hole condition was relatively low. In contrast, the hole expansion perfor­ mance of dual phase steel and austenitic stainless steel with laser cutting * Corresponding authors at: Institute of Forming Technology and Equipment, School of Materials Science and Engineering, Shanghai Jiao Tong University, Shanghai 200030, China. E-mail addresses: [email protected] (X. Zhuang), [email protected] (Z. Zhao). https://doi.org/10.1016/j.mtcomm.2025.111749 Received 25 November 2024; Received in revised form 18 January 2025; Accepted 27 January 2025 Available online 27 January 2025 2352-4928/© 2025 Elsevier Ltd. All rights are reserved, including those for text and data mining, AI training, and similar technologies. Q. Li et al. Materials Today Communications 43 (2025) 111749 hole was better. Li et al. [14] studied the effect of inner hole cutting process on the expansion performance of AHSSs. The HER of AHSSs with punched hole was significantly lower than that with milled hole and laser cutting hole. Vibration-assisted forming is an emerging plastic-processing tech­ nology developed in recent years. By applying a certain amplitude and frequency of vibration during material formation, it is possible to reduce the forming force and improve the forming limit. The microstructures such as dislocations, are changed by the superposition of vibrations, affecting their mechanical behaviour. Dutta et al. [15] found that the dislocation density of low-carbon steel decreases after ultrasonic vi­ bration treatment. This is the result of long-range movement and the annihilation of dislocations promoted by ultrasonic vibrations. Meng et al. [16] conducted vibration-assisted tensile tests of low-carbon steel with different amplitudes on ultrathin high-temperature alloy plates to explore their effect on the mechanical properties and microstructure evolution. The vibration caused a significant change in the texture orientation, with an increase in elongation from 20.7 % to 25.5 %. Lin et al. [17]applied low frequency vibration during the upsetting test of titanium alloy and studied the deformation mechanism. The results showed that vibration promoted dislocation movement and grain rota­ tion, resulting in dislocation annihilation in the shear bands. More ho­ mogenous deformation occurred with low-frequency vibration assisted upsetting compared with conventional static upsetting. Currently, most studies have focused on ultrasonic vibration-assisted forming. Compared to ultrasonic vibration, low-frequency vibration technology [18] has a greater vibration force and is used in the formation and production of large parts. Research on low-frequency vibration-assisted forming has mainly focused on aluminium alloys, copper alloys, titanium alloys, and low-carbon steels with low strength, while little research has been conducted on the increasing demand for AHSS. The effect of low-frequency vibration-assisted forming on improving the forming limit is consistent with the shortcomings of AHSS reported in previous research, such as easy cracking at the edges and low expansion perfor­ mance. However, there are several possibilities for combining low-frequency vibration-assisted and AHSS forming. To better understand the coupling mechanisms between lowfrequency vibration and the deformation behaviour, and improve the expansion performance of AHSS, low-frequency vibration-assisted hole expansion (LFVHE) test was performed on QP980 in this study. In addition, various fabrication methods including wire cutting and laser cutting were adopted for the inner hole of QP980. To explain the hole expansion performance, the microstructure evolution characteristics of QP980 was investigated by EBSD, TEM, and nanoindentation. Finally, the hole expansion performance and microstructure evolution of QP steel in LFVHE were obtained. Fig. 1. Microstructure of QP980. Fig. 2. Mechanical properties of QP980 in different directions. hole is uniform during the loading process, and the influence of anisotropy on hole expansion performance was not considered in LFVHE. 2.2. Experimental setup The LFVHE experimental platform is shown in Fig. 3(a) and consists of three parts: a low-frequency vibration system, a hole expansion de­ vice, and a universal testing machine. The vibration superimposed during the hole expansion process is generated by a low-frequency vi­ bration system, which is an electro-hydraulic excitation system composed of three parts: a vibration control station, a hydraulic unit, and a vibration hydraulic cylinder. The input signal from the control station controls the servo valve in the hydraulic station to change the inlet and outlet oil volumes. The vibration amplitude is generated by the change of the oil quantity and the vibration frequency is modified by the commutation frequency of oil. The maximum response frequency of the servo valve is 100 Hz, and the maximum amplitude of the excitation cylinder is 2 mm. The maximum vibration excitation force generated by the hydraulic cylinder is 200 kN. In the tests, the vibration cylinder is equipped with displacement sensors and external Hantek software to capture and measure the real amplitude and frequency, ensuring the accuracy of the actual amplitude and frequency. The accuracy of the displacement sensor is ± 0.5 μm. The hole-expansion device includes a die, blank holder, and punch. A conical punch with a 60◦ cone angle is connected to a vibrating hy­ draulic cylinder. In the experimental process, the amplitude and fre­ quency applied to the punch are adjusted through a control station to provide low-frequency vibrations in the vertical direction. The beam of 2. Material and experimental setup 2.1. Material The chemical compositions of received QP980 steel sheet is shown in Table 1, and the thickness of the sheet is 1.4 mm. QP980 is composed mainly of ferrite (F), martensite (M), and retained austenite (Ar), as shown in Fig. 1(a). The majority of the microstructure of QP980 is ferrite and martensite, and retained austenite is dispersed on the matrix of ferrite and martensite. The stress-strain curves of QP980 along the 0◦ , 45◦ , and 90◦ rolling directions are shown in Fig. 2. It can be found that the anisotropy is not significant. In hole expansion tests, the stress at the edge of the inner Table 1 Chemical composition of QP980 (wt%). C Mn Si P S Ti Fe 0.20 2.04 1.57 0.008 0.002 0.0061 Bal. 2 Q. Li et al. Materials Today Communications 43 (2025) 111749 Fig. 3. The experimental platform of LFVHE: (a) experimental platform; (b) schematic of LFVHE. the universal testing machine is effectively connected to the die, and moves downwards together. The sheet specimen is placed between die and blank holder. During the tests, the position of punch remains un­ changed. The die contacts sheet specimen and drives the sheet specimen and the blank holder to move downwards together. The nitrogen gas springs are placed between blank holder and spring positioning plate. Die, sheet specimen and blank holder move downwards to compress the nitrogen gas springs, and the nitrogen gas springs are compressed to provide blank holder force. A schematic of the LFVHE is shown in Fig. 3 (b). As previously stated, it is necessary to determine the additional thermal effect generated by vibration. Because of the inconvenience of measuring temperature during the hole expansion process and the fact that the inner hole is subjected to uniaxial tensile stress[19], a uniaxial tensile test is used. The vibration-assisted tensile testing platform is shown in Fig. 4(a). A thermal infrared imager was used to determine the temperature during the tensile testing. And the temperature of the specimen throughout the process was recorded by a signal collection equipment. A tensile speed of 2 mm/min was set, and the testing ma­ chine and thermal imager recordings started simultaneously. A low-frequency vibration with a frequency of 30 Hz and an amplitude of 0.243 mm was superimposed when the deformation time was 60 s. The maximum temperature of the specimen was recorded every 30 s. Room temperature was approximately 22 ℃ and the time interval between the two groups of experiments did not exceed 3 min. The temperature of the specimens is illustrated in Fig. 4(b). Part of mechanical energy will be converted into thermal energy during plastic deformation, which causes an increase in the surface temperature of the tensile specimen. More­ over, an additional slight increase of 2 ℃ is induced by the superposition of vibrations, indicating that vibrations does not produce a significant thermal effect. The impact of the temperature on the HER and micro­ structure evolution was not considered in the LFVHE. 2.3. Experimental procedure The specimen used in this study is circular, with a diameter of 180 mm and an inner hole in the centre with a diameter of 10 mm, as shown in Fig. 5. Both wire cutting and laser cutting were used to ma­ chine the inner hole. Wire cutting was performed with a slow wire using electric discharge wire-cutting equipment. The laser cutting equipment has a power of 700 W, a cutting nozzle length of 1.5 mm, and a focal length of 2.0 mm. Nitrogen gas protection was used during cutting. When the inner hole of the specimen was close to the punch (not in contact), the testing machine displacement was reset to the initial displacement point during the experiment. The loading speed of the testing machine was set to 2 mm/min and the vibration equipment was initiated simultaneously. The specimen was loaded with the punch Fig. 5. Specimens of LFVHE. Fig. 4. Temperature measurement: (a) experimental platform; (b) temperature variation. 3 Q. Li et al. Materials Today Communications 43 (2025) 111749 downward. When obvious cracks penetrated the thickness direction of the inner hole, the universal test machine and low-frequency vibration stopped simultaneously. The expansion performance is generally evaluated using the HER, which is related to the diameter of the pre-processed hole and the diameter of the inner hole after expansion, as follows [20]: HER = area at the edge of the inner hole is small and curved, making it difficult to test. Therefore, in this study, the retained austenite statistics were based on the EBSD results, and the average phase content was deter­ mined. The TEM samples were sectioned into discs with a diameter of 3 mm, and then mechanically ground to a thickness of 80–100 μm. The prepared samples were subsequently polished to perforation by using a twin-jet electro-polishing. The microstructure morphologies of the specimens after LFVHE were analysed using Talos F200X G2 TEM. Finally, a Hysitron TI-950 nanomechanical test system was used for the nanoindentation test. A 4 × 4 indentation matrix was pressed at an indentation distance of 4 μm in the testing area. The nanoindentation experiment used Berkovich diamond probe, with a maximum pressure of 10 mN and a maximum depth of 5 μm. The curvature radius of the diamond probe is approximately 100 nm. The test specimen was vi­ bration polished to remove the retained surface stress before the test to ensure the accuracy of the experiment. A maximum load of 10000 μN was maintained during the test, and the load-unload curve and hardness value for each indentation were obtained. Two different micro areas at the edge of the inner hole were selected for testing. Afterwards, EBSD was used to observe the indentation area. The martensite and ferrite were distinguished by grain morphology. Ferrite appears as a block, with a large volume and no fixed shape of the grain boundaries. The martensite morphology was parallel lath-shaped and the indentation was completely pressed inside the ferrite or martensite. The hardness at the point was taken as the hardness of the ferrite or martensite. The testing results of each phase were averaged based on three indentations to ensure the repeatability of the results, and the standard deviation of the results was marked with error bars [21,22]. Df − D0 × 100% D0 where Df represents the diameter of the inner hole after fracture, and D0 represents the diameter of the pre-processed hole, which in the experi­ ment is uniformly 10 mm. The vibration frequency was uniformly set to 30 Hz with four selected amplitudes: 0.062, 0.125, 0.165, and 0.243 mm. And the amplitudes and frequency are independent of the thickness of sheet. To ensure the accuracy of the expansion performance, the tests were repeated three times for each vibration amplitude. To explain the changes in the HER of QP980, microhardness, EBSD, TEM, and nanoindentation tests were performed to determine the microstructural evolution of LFVHE. A microhardness tester was used to test the hardness distribution of the inner hole for different hole-cutting processes. The indenter load was 300 gf, and the pressure holding time was 10 s. Each sample was marked with three points in different areas, and the final hardness was taken as the average value. EBSD was used to determine the changes in the dislocation density, grain boundary dis­ tribution, and phase distribution with different hole expansion times and vibration conditions. TEM and nanoindentation tests were used to observe the distribution of dislocations and the microhardness of different grains, respectively. Two different groups of vibration times were set to study the microstructural evolution process of the QP steel during the LFVHE process, two different groups of vibration times were set. The first group of tests was timed for 240 s and the second group was timed for 360 s, and the deformation of the inner hole edge at these times was defined as ε1 and ε2 (ε1 < ε2 ), without any fracture. To ensure the consistency of strain in each group of experiments, timing starts from the contact of the punch with the inner hole. The testing time for the two groups was the loading time, which is 240 s and 360 s respectively. Small pieces along the inner hole were cut using wire cutting equipment, and the cutting positions were relatively random because of the absence of anisotropy, as shown in Fig. 6(a) and (b). Fig. 6(c) shows that the area of the EBSD, TEM, and the nano­ indentation test is the edge of the inner hole. For the EBSD test, the NOVA Nano SEM 230 electron microscope was used, with an accelerated voltage of 20 kV, an amplification factor of 8000 times, a scanning step size of 0.05 μm and a scanning area of 15 μm × 15 μm. Azteccrystal and Channel 5 software were used for data processing. Each group of samples was tested in three areas, and the relevant values were aver­ aged. In addition, the content and distribution of the retained austenite in the LFVHE were illustrated the effect of low-frequency vibrations on the TRIP effect. Generally, the retained austenite content in QP980 is determined by X-ray diffraction (XRD). However, in the experiment, the 3. Results and discussion 3.1. The influence of fabrication methods on the microstructure of the inner hole The microstructure of the inner hole edges of QP980 obtained by wire and laser cutting are shown in Fig. 7(a) and (b), respectively. The blue area represents the BCC phase, which includes ferrite and martensite. The red area represents the FCC phase, which is the retained austenite (6.4 %) in Fig. 7(a). The retained austenite distributed on the ferrite matrix consisted of large block-shaped particles (black arrows) and small particles (yellow arrows), and distributed on the martensite matrix was plot-shaped (green arrows) with the smallest size and dispersion distribution. In the microstructure of QP980 with laser cut hole, the retained austenite content is less than 1 %, as shown in Fig. 7 (b). This is because the removal of the heat source after laser cutting led to a rapid quenching of the inner hole by solid heat transfer. There is fine plate-shaped quenched martensite around the inner hole, and the TRIP effect hardly occurs during deformation. Therefore, wire cutting largely retains the original microstructure of QP980[23]. QP980 with wire cut hole, was used to test the microstructure evolution in LFVHE. Fig. 6. Specimen after deformation: (a) hole expansion at ε1 ; (b) top view of testing area; (c) test area. Fig. 7. Microstructure of QP980 of the inner hole: (a) wire cutting; (b) laser cutting. 4 Q. Li et al. Materials Today Communications 43 (2025) 111749 The QP980 sample were selected along the rolling direction for microhardness testing. The starting point was the edge of the inner hole, and then the testing area was taken every 25 μm along the rolling di­ rection, as shown in Fig. 8(a). Three points were marked in each area, and the average value was considered the final hardness value. The microhardness distributions of the inner holes are shown in Fig. 8(b). The original microhardness of QP980 is 332.52 HV, and the micro­ hardness with wire cut hole is 330.6 HV, which is relatively consistent. As the distance from the inner hole increased, the hardness fluctuates between 325 HV and 340 HV without a significant increase. In addition, the microhardness of QP980 with laser cut hole is 495.5 HV, which is much higher than the original microhardness of 303.27 HV. This is because a large amount of brittle and hard-quenched martensite significantly increases the hardness. This indicates that the laser cutting process has a significant hardening behaviour, whereas wire cutting does not. Fig. 9. HER of QP980 with different vibration amplitudes. 3.2. Hole expansion performance of QP980 vibration amplitudes is shown in Fig. 11. Dislocations within the ferrite grains at ε1 without vibration are rare, as shown in Fig. 11(a). In addi­ tion, the blue stripes, representing a high GND density, are distributed in the lath martensite. More blue stripes are produced in the ferrite grains with an amplitude of 0.062 mm, as illustrated in Fig. 11(b). The red areas in the ferrite grains decrease significantly, while the yellow areas and blue stripes increase significantly at a vibration amplitude of 0.243 mm (Fig. 11(c)). The proliferation of dislocations is promoted obviously after the superposition of vibration with an amplitude of 0.243 mm during the early deformation in LFVHE. The partial area representing low dislocation density is replaced by the yellow area with higher GND density in the ferrite at ε2 without vibration (Fig. 11(d)). The blue stripes are mostly distributed in the ferrite grains with an amplitude of 0.062 mm (Fig. 11(e)), indicating that there is an increase in dislocations within ferrite grains. The ferrite grains marked in Fig. 11(f) appears dark red and have a low GND density with an amplitude of 0.243 mm, whereas the surrounding martensite lath appears green or blue and has a high dislocation density. Compared with ε1 (Fig. 11(c)), the low-density GND region of ε2 is mainly concentrated in ferrite grains with an amplitude of 0.243 mm. By combining the EBSD measurements and the relevant dislocation parameters, the GND density of the BCC phase of QP980 is obtained, as shown in Fig. 12. The GND density of ε1 without vibration is 11.78 × 1014 /m2 and the GND density with a small amplitude of 0.062 mm is higher than that without vibration at ε1 and ε2 . Moreover, the dislocation proliferation is further promoted by an increase in the vibration time. The density of GND increased significantly with an amplitude of 0.243 mm, reaching 21.61 × 1014 /m2 at ε1 . Compared to ε1 , the GND density decreased at ε2 . The proliferation of dislocations is promoted with a large amplitude of 0.243 mm in the early stage of In Fig. 9, the HER of QP980 with wire cut hole is 51.0 % without vibration, while the HER with laser cut hole decreases to 29.1 %. This is because crack initiation and growth are promoted by the hard and brittle quenched martensite of the inner hole; thus, the hole expansion per­ formance significantly reduces. The HER of QP980 with wire cut hole with an amplitude of 0.062 mm increases to 54.7 %, whereas the HER decreases with amplitudes of 0.125, 0.165, and 0.243 mm. At the maximum amplitude of 0.243 mm, the HER decreases by 22.0 %. The HER of QP980 with laser cut hole gradually decreases with the increasing amplitude. The HER increases to 34.7 % at an amplitude of 0.062 mm and decreases to 25.8 % at an amplitude of 0.243 mm. Therefore, increasing the vibration amplitude causes a decrease in the HER of QP980 with a vibration frequency of 30 Hz. To further determine the effect of low-frequency vibration on the hole expansion performance of QP980, low-frequency vibration with the same amplitudes were superimposed during uniaxial tension tests. Vi­ bration was superimposed during tensile testing from a strain of 0.03 until fracture. Stress-strain curves and elongation of QP980 with different amplitudes are shown in Fig. 10 and Table2, respectively. Compared to conventional tension, the elongation of QP980 increases to 24.2 % with a 0.062 mm amplitude, and elongation decreases with the increasing vibration amplitude. The elongation and HER of QP980 exhibit the same pattern as the amplitude changes. 3.3. The microstructure evolution of QP980 in LFVHE 3.3.1. Dislocation evolution The proportions of ferrite and martensite in QP980 are more than 90 %, and these are the main deformation phases in LFVHE. The dis­ tribution of GND in the BCC phase (ferrite and martensite) with different Fig. 8. Microhardness of QP980: (a) test area; (b) microhardness. 5 Q. Li et al. Materials Today Communications 43 (2025) 111749 Fig. 10. Stress-strain curves of QP980 with different amplitudes: (a) 0.062 mm; (b) 0.125 mm; (c) 0.165 mm; (d) 0.243 mm. LFVHE, and significant dislocation annihilation may occur with increasing strain. The additional energy generated by the vibration can reduce the activation energy of the dislocation source [24] in the LFVHE, signifi­ cantly increasing the dislocation density. Increasing amplitudes is beneficial for dislocation proliferation owing to the high vibration en­ ergy. The dislocation density with an amplitude of 0.243 mm is higher Table 2 Elongation of QP980 with different vibration amplitudes. Amplitude/mm 0 0.062 0.125 0.165 0.243 Elongation/% 23.3 24.2 23.5 22.3 19.5 Fig. 11. GND distribution at ε1 : (a) 0 mm; (b) 0.062 mm; (c) 0.243 mm and GND distribution at ε2 : (d) 0 mm; (e) 0.062 mm; (f) 0.243 mm. 6 Q. Li et al. Materials Today Communications 43 (2025) 111749 reduces dislocation density in low-frequency vibration assisted low carbon steel tensile tests. Lin et al.[26] investigated that vibration pro­ motes dislocation motion and grain rotation, result in the annihilation of dislocations within the shear band in the low-frequency vibration assisted titanium alloy upsetting tests. 3.3.2. TRIP effect The distribution of the phases is shown in Fig. 14. The retained austenite is large block, granular-shaped in the ferrite matrix and spotshaped in the martensite matrix at ε1 without vibration (Fig. 14(a)). The block-shaped retained austenite at ε1 transforms partially with a vibration amplitude of 0.062 mm (Fig. 14(b)), resulting in a reduced volume fraction compared with that without vibration. Only the spotshaped austenite remains in the martensite matrix with a vibration amplitude of 0.243 mm. The transformation of retained austenite is promoted after the superimposition of low-frequency vibration, and the phenomenon is more evident at the large amplitude of 0.243 mm. The volume fraction of retained austenite (VFRA) of inner hole at different amplitudes is shown in Fig. 15. The VFRA without vibration at ε1 is 2.60 % and decreases to 2.00 % with an amplitude of 0.062 mm. The retained austenite almost disappeared when the amplitude increased to 0.243 mm. The superposition of low-frequency vibrations is conducive to the transformation of retained austenite into martensite, and increasing the amplitude promotes this effect. The transformation of residual austenite usually depends on high energy density areas such as grain boundaries. The distribution and proportion of grain boundaries of QP980 are shown in Fig. 16. The low angle grain boundary (LAGB) is defined as the difference in orientation between consecutive grains of 2◦ to 15◦ , and the high angle grain boundary (HAGB) is defined as the difference in orientation greater than 15◦ . Only a small number of LAGB appeared without vibration (18.9 %), as shown in Fig. 16(a). There is a small increase in the proportion of LAGB with a vibration amplitude of 0.062 mm (Fig. 16(b)). While a large number of dense LAGBs forms in the ferrite grains with a vibration amplitude of 0.243 mm (Fig. 16(c)), corresponding to 37.4 %. The difficulty of the retained austenite phase transformation is related to its size [27]. The retained austenite in a large block is unstable [28] and easily transforms into martensite during the early stages of deformation [29]. Compared with the large block, the retained austenite of the granular on the ferrite matrix is stable and transforms to martensite. In addition, the plot-shaped retained austenite in the martensite matrix is the most stable and shows almost no trans­ formation. It is because that plot-shaped retained austenite is sur­ rounded by lath martensite with high yield strength. Therefore, the transformation is restrained [30,31]. The transformation of the retained austenite in large blocks is facilitated by the proliferation of dislocations, resulting in a significant reduction in VFRA. In addition, the transformation of granular retained austenite in the ferrite matrix is related to substructures such as LAGB. The generated dislocations arrange into dislocation walls and eventually evolve into Fig. 12. GND density of QP980 with different vibration amplitudes. than that of 0.062 mm at ε1 . But as the vibration time increases, the vibration amplitudes have different effects on the dislocation. Compared to martensite, ferrite is more prone to deformation and the proliferation and annihilation of dislocations mainly occur within the ferrite grains. Dislocations acquire a greater migration distance and mobility with an amplitude of 0.243 mm. The probability of a negative dislocation meeting increases within the ferrite grains, which promotes the annihilation of disloca­ tions. The rapid proliferation and accumulation of dislocations in the early stage of deformation also provide a high probability for positive and negative dislocations to meet. The annihilation of dislocations leads to a decrease in GND density during the LFVHE process from ε1 to ε2 . To further prove the behaviour of dislocation annihilation, the microstructure morphology of martensite and ferrite at ε2 were tested by TEM. More dislocations exist in the lath martensite and grain boundaries at ε2 without vibration (Fig. 13(a)), and there is a difference in dislo­ cation density between the lath martensite and the ferrite grains. In Fig. 13(b), it can be observed that the dislocation density inside ferrite grains increases with an amplitude of 0.062 mm. Similar to the EBSD test results, the proliferation of dislocations within the ferrite grains is promoted by the superposition of vibration at ε2 . The lath martensite and ferrite grain boundary contained a lot of dislocations with a vibration amplitude of 0.243 mm (Fig. 13(c)). However, the dislocation density inside the adjacent ferrite grains is relatively low. Comparing to the case without vibration, the difference in dislocation density between the martensite and adjacent ferrite increased with a vibration amplitude of 0.243 mm, attributing to the annihilation of dislocations within the ferrite grains. This result corre­ sponds to the GND density mentioned above. The phenomenon of dislocation annihilation in low-vibration assisted forming has also been discovered in previous studies. Meng et al.[25] found that the super­ position of vibration promotes the annihilation of dislocations and Fig. 13. Microstructure morphology of the inner hole edge at ε2 : (a) 0 mm; (b) 0.062 mm; (c) 0.243 mm. 7 Q. Li et al. Materials Today Communications 43 (2025) 111749 Fig. 14. Distribution of phases at ε1 : (a) 0 mm; (b) 0.062 mm; (c) 0.243 mm. diagram at ε1 with an amplitude of 0.243 mm are presented in Fig. 17 (a), where the white stripe is LAGB and the black stripe is HAGB. Several new grain boundaries are found around the retained austenite in the granular area marked by the yellow arrow. Massive new LAGB Fig. 15. Volume fraction of retained austenite with different amplitudes. Fig. 17. Transformation process of granular retained austenite: (a) diagram of phase distribution and grain boundary distribution; (b) diagram of transformation. LAGB [32]. The phase distribution and grain boundary distribution Fig. 16. Distribution and proportion of grain boundaries of QP980 at ε1: (a) 0 mm; (b) 0.062 mm; (c) 0.243 mm and (d) proportions of LAGB and HAGB. 8 Q. Li et al. Materials Today Communications 43 (2025) 111749 generated in the ferrite grains promoted the granular transformation of retained austenite, as shown in Fig. 17(b). Owing to the proliferation of dislocations and the generation of new grain boundaries with a vibration amplitude of 0.243 mm, the TRIP effect occurs in the retained austenite which have the block and granular. The retained austenite within the martensite matrix does not transform. Additional heat can be generated by dislocation proliferation and the TRIP effect [33] which cause a temperature increase. This explains the small temperature increase of 1–2 C◦ after the superposition of vibra­ tions in Fig. 4(b) and proves that the low-frequency vibrations hardly generated additional thermal effects. expansion performance of QP980 depends on the deformation behav­ iour of ferrite and martensite in LFVHE. The superposition of lowfrequency vibration has an impact on dislocations within ferrite and martensite grains, and the relationship between dislocation and HER needs further verification. The nanoindentation tests were performed on the edges of inner holes with different amplitudes at ε2 , and the hardness of ferrite and martensite was obtained in Fig. 18. In Fig. 18(a), ferrite is surrounded by white lines and lath martensite is surrounded by orange lines. The indentation points inside the grains are marked by yellow triangles. The load-unload curves of the test area at ε2 are shown in Fig. 18(b)~(d), and the average hardness of two phases is listed in Table 3. The proliferation of dislocations with an amplitude of 0.062 mm increases the hardness of ferrite and martensite. Compared to without vibration, the hardness of ferrite is closer to that of martensite with an amplitude of 0.062 mm. Compared to without vibration, the hardness ratio between ferrite and 3.4. The relationship between microstructure and HER of QP980 Ferrite and martensite account for over 90 % of the proportion in QP steel, and retained austenite has almost transformed before ε2. The hole Fig. 18. Nanoindentation test results: (a) EBSD schematic diagram; (b) load-unload curve without vibration; (c) load-unload curve with an amplitude of 0.062 mm; (d) load-unload curve with an amplitude of 0.243 mm; (e) average hardness values. 9 Q. Li et al. Materials Today Communications 43 (2025) 111749 Declaration of Competing Interest Table 3 Average hardness of ferrite and martensite under different vibration conditions. Hardness/GPa 0 mm 0.062 mm 0.243 mm Ferrite Martensite Ferrite/Martensite 4.75 5.71 0.832 5.25 6.06 0.866 4.86 6.43 0.755 All authors disclosed no relevant relationships. Acknowledgements This research was supported by the National Natural Science Foun­ dation of China (grant nos. 52375352) and Shanghai Outstanding Aca­ demic Leaders Plan (21XD1422000). martensite decreases to 0.755 with an amplitude of 0.243 mm. The hardness difference between the ferrite and martensite has a significant impact on the HER. An increase in the hardness difference is not conducive to coordinated deformation between grains. In contrast, reducing the hardness difference improves HER. This phenomenon has been reported previously. Taylor et al.[34] conducted nanoindentation experiments on DP980 and found that the HER increased with a decrease in the hardness ratio of martensite and ferrite. Kohei et al. [35] studied the crack propagation through the interface of martensite and ferrite during the hole expansion and tension of a dual-phase steel flange and confirmed that the difference in hardness between the two phases affected the formability of the flanges. Kim et al. [36] believed that the change in the HER was significantly related to the continuity of martensite and the local deformation of ferrite. The annihilation of dislocations in ferrite grains with an amplitude of 0.243 mm causes a decrease in hardness of ferrite. The decrease in hardness of ferrite leads to a large hardness difference between ferrite and martensite, decreasing the HER of QP980. The hardness difference between ferrite and martensite decreases, and the homogeneous distribution promotes the uniform deformation of the inner hole with an amplitude of 0.062 mm, improving HER. Data availability Data will be made available on request. References [1] Y. Qiao, Z. Zheng, H. Yang, J. Long, P. Han, Recent progress in microstructural evolution, mechanical and corrosion properties of medium-Mn steel, J. Iron Steel Res. Int. 30 (2023) 1463–1476, https://doi.org/10.1007/s42243-023-00974-w. [2] D.C. Ramachandran, A.R.H. Midawi, M. Shojaee, O. Sherepenko, H. GhassemiArmaki, E. Biro, A comprehensive evaluation of tempering kinetics on 3rd generation advanced high strength steels, Materialia 26 (2022) 101644, https:// doi.org/10.1016/j.mtla.2022.101644. [3] S.K. Paul, Correlation between hole expansion ratio (HER) and notch tensile test, Manuf. Lett. 20 (2019) 1–4, https://doi.org/10.1016/j.mfglet.2019.02.003. [4] J. He, G. Han, S. Li, D. Zou, To correlate the phase transformation and mechanical behavior of QP steel sheets, Int. J. Mech. Sci. 152 (2019) 198–210, https://doi.org/ 10.1016/j.ijmecsci.2019.01.003. [5] S.K. Paul, The effect of deformation gradient on necking and failure in hole expansion test, Manuf. Lett. 21 (2019) 50–55, https://doi.org/10.1016/j. mfglet.2019.08.004. [6] S. Xu, S. Li, S. Wang, J. Gao, R. Cao, Q. Feng, H. Li, X. Mao, Research status and prospect of direct strip casting manufactured low-carbon microalloyed steel, J. Iron Steel Res. Int. 29 (2022) 17–33, https://doi.org/10.1007/s42243-021-00739-3. [7] M. Chinara, S.K. Paul, S. Chatterjee, S. Mukherjee, Experimental investigation of hole expansion ratio for automotive-grade steels, Proc. Inst. Mech. Eng. B J. Eng. 237 (2023) 1283–1291, https://doi.org/10.1177/09544054221121892. [8] Y. Ma, Y. Yu, P. Geng, R. Ihara, K. Maeda, R. Suzuki, T. Suga, N. Ma, Fracture modeling of resistance spot welded ultra-high-strength steel considering the effect of liquid metal embrittlement crack, Mater. Des. 210 (2021) 110075, https://doi. org/10.1016/j.matdes.2021.110075. [9] S.K. Paul, Non-linear correlation between uniaxial tensile properties and shearedge hole expansion ratio, J. Mater. Eng. Perform. 23 (2014) 3610–3619, https:// doi.org/10.1007/s11665-014-1161-y. [10] O.R. Terrazas, K.O. Findley, C.J. Van Tyne, Influence of martensite morphology on sheared-edge formability of dual-phase steels, ISIJ Int. 57 (2017) 937–944, https:// doi.org/10.2355/isijinternational.ISIJINT-2016-602. [11] X. Chen, H. Jiang, Z. Cui, C. Lian, C. Lu, Hole expansion characteristics of ultra high strength steels, Procedia Eng. 81 (2014) 718–723, https://doi.org/10.1016/j. proeng.2014.10.066. [12] L. Xu, F. Barlat, M.G. Lee, Hole expansion of twinning-induced plasticity steel, Scr. Mater. 66 (2012) 1012–1017, https://doi.org/10.1016/j.scriptamat.2012.01.062. [13] B.M. Hance, R.J. Comstock, D.K. Scherrer, The influence of edge preparation method on the hole expansion performance of automotive sheet steels, SAE Int. 01 (2013) 1167, https://doi.org/10.4271/2013-01-1167. [14] D.J. Branagan, A.E. Frerichs, B.E. Meacham, S. Cheng, A.V. Sergueeva, New mechanisms governing local formability in 3rd generation AHSS, SAE Int. 01 (2017) 1704, https://doi.org/10.4271/2017-01-1704. [15] R.K. Dutta, R.H. Petrov, R. Delhez, M.J.M. Hermans, I.M. Richardson, A.J. Böttger, The effect of tensile deformation by in situ ultrasonic treatment on the microstructure of low-carbon steel, Acta Mater. 61 (2013) 1592–1602, https://doi. org/10.1016/j.actamat.2012.11.036. [16] B. Meng, B. Cao, M. Wan, C. Wang, D. Shan, Constitutive behavior and microstructural evolution in ultrasonic vibration assisted deformation of ultrathin superalloy sheet, Int. J. Mech. Sci. 157–158 (2019) 609–618, https://doi.org/ 10.1016/j.ijmecsci.2019.05.009. [17] J. Lin, C. Pruncu, L. Zhu, J. Li, Y. Zhai, L. Chen, Y. Guan, G. Zhao, Deformation behavior and microstructure in the low-frequency vibration upsetting of titanium alloy, J. Mater. Process Technol. 299 (2022) 117360, https://doi.org/10.1016/j. jmatprotec.2021.117360. [18] Y. Zhang, B. Wu, E. Gao, L. Shui, Z. Liu, Observation of speeding growth of metal nanowires by ultra-low frequency micro-vibration assisted superplastic nanomolding, Mater. Lett. 283 (2021) 128890, https://doi.org/10.1016/j. matlet.2020.128890. [19] J.J. Kim, Q.T. Pham, Y.S. Kim, Thinning prediction of hole-expansion test for DP980 sheet based on a non-associated flow rule, Int. J. Mech. Sci. 191 (2021) 106067, https://doi.org/10.1016/j.ijmecsci.2020.106067. [20] S.K. Paul, A critical review on hole expansion ratio, Materialia 9 (2020) 100566, https://doi.org/10.1016/j.mtla.2019.100566. [21] H. Farivar, S. Richter, M. Hans, A. Schwedt, U. Prahl, W. Bleck, Experimental quantification of carbon gradients in martensite and its multi-scale effects in a DP 4. Conclusions An electrohydraulic excitation device was used to investigate the effect of low-frequency vibrations on the hole expansion performance of QP steel. The hole expansion performance and microstructure evolution of QP steel in LFVAT were obtained. The following conclusions are drawn: 1) Compared with wire cutting, the HER of QP980 with laser cut hole reduces significantly, and the TRIP effect does not occur. The HER of QP980 with wire cut hole and laser cut hole exhibit similar patterns with change of vibration amplitude in LFVHE. Increasing the vibra­ tion amplitude causes a decrease in the HER with a vibration fre­ quency of 30 Hz. 2) The TRIP effect of QP980 is promoted in LFVHE owing to the pro­ liferation of dislocations after the superposition of vibration. The large block-shaped retained austenite transforms to martensite in the early stages of LFVAT. In addition, dislocation proliferation pro­ motes the form of LAGB and the transformation of residual austenite on the ferrite matrix. 3) The vibration amplitude affects HER of QP steel by influencing the hardness difference between ferrite and martensite. The proliferation of dislocations leads to an increase in hardness of ferrite with an amplitude of 0.062 mm, improving HER. As the amplitude increases to 0.243 mm, the annihilation of dislocations within the ferrite grains increases the hardness difference between ferrite and martensite, which is unfavourable for improving HER. CRediT authorship contribution statement Zhang Wen: Methodology, Investigation. Li Qi: Writing – original draft, Methodology, Formal analysis. Yang Huachao: Methodology, Formal analysis. Zhuang Xincun: Resources, Funding acquisition. Zhao Zhen: Supervision. Sun Han: Methodology. 10 Q. Li et al. Materials Today Communications 43 (2025) 111749 steel, Mater. Sci. Eng. A 718 (2018) 250–259, https://doi.org/10.1016/j. msea.2018.01.106. [22] J. Wang, W. Li, X. Zhu, L. Zhang, Effect of martensite morphology and volume fraction on the low-temperature impact toughness of dual-phase steels, Mater. Sci. Eng. A 832 (2022) 142424, https://doi.org/10.1016/j.msea.2021.142424. [23] M. Zhou, Y. Li, Q. Hu, X. Li, J. Chen, Investigations on edge quality and its effect on tensile property and fracture patterns of QP980, J. Manuf. Process 37 (2019) 509–518, https://doi.org/10.1016/j.jmapro.2018.12.028. [24] Y. Xu, X. Zhuang, W. Zhang, Q. Li, Z. Zhao, Mechanical behaviors and microstructure characteristics of W-tempered and peak-aged 7075 alloy sheets under low frequency vibration–assisted tension, Mater. Sci. Eng. A 833 (2022) 142338, https://doi.org/10.1016/j.msea.2021.142338. [25] D. Meng, X. Zhao, S. Zhao, Q. Han, Effects of vibration direction on the mechanical behavior and microstructure of a metal sheet undergoing vibration-assisted uniaxial tension, Mater. Sci. Eng. A 743 (2019) 472–481, https://doi.org/10.1016/ j.msea.2018.11.115. [26] J. Lin, C. Pruncu, L. Zhu, J. LI, Y. Zhai, L. Chen, Y. Guan, G. Zhao, Deformation behavior and microstructure in the low-frequency vibration upsetting of titanium alloy, J. Mater. Process Technol. 299 (2022) 117360, https://doi.org/10.1016/j. jmatprotec.2021.117360. [27] J. Min, L.G. Hector, L. Zhang, J. Lin, J.E. Carsley, L. Sun, Elevated-temperature mechanical stability and transformation behavior of retained austenite in a quenching and partitioning steel, Mater. Sci. Eng. A 673 (2016) 423–429, https:// doi.org/10.1016/j.msea.2016.07.090. [28] B.V.N. Rao, M.S. Rashid, Direct Observations of deformation-induced retained austenite transformation in a vanadium-containing dual-phase steel, Mater. Charact. 39 (1997) 435–453, https://doi.org/10.1016/s1044-5803(97)00156-3. [29] A. Sierra-Soraluce, G. Li, M.J. Santofimia, J.M. Molina-Aldareguia, A. Smith, M. Muratori, I. Sabirov, Effect of microstructure on tensile properties of quenched and partitioned martensitic stainless steels, Mater. Sci. Eng. A 864 (2023) 144540, https://doi.org/10.1016/j.msea.2022.144540. [30] P.J. Jacques, J. Ladrie`re, L. Ladrie`re, F. Delannay, On the Influence of Interactions between Phases on the Mechanical Stability of Retained Austenite in Transformation-Induced Plasticity Multiphase Steels, Met. Mater. Trans. A 32 (2001) 2759–2768, https://doi.org/10.1007/s11661-001-1027-4. [31] X. Xiong, B. Chen, M. Huang, J. Wang, L. Wang, The effect of morphology on the stability of retained austenite in a quenched and partitioned steel, Scr. Mater. 68 (2013) 321–324, https://doi.org/10.1016/j.scriptamat.2012.11.003. [32] S. Kim, K. Kang, S.Y. Kim, Dynamic drags acting on moving defects in discrete dispersive media: from dislocation to low-angle grain boundary, J. Mech. Phys. Solids 145 (2020) 104166, https://doi.org/10.1016/j.jmps.2020.104166. [33] A. Das, S. Tarafder, Experimental investigation on martensitic transformation and fracture morphologies of austenitic stainless steel, Int. J. Plast. 25 (2009) 2222–2247, https://doi.org/10.1016/j.ijplas.2009.03.003. [34] M.D. Taylor, K.S. Choi, X. Sun, D.K. Matlock, C.E. Packard, L. Xu, F. Barlat, Correlations between nanoindentation hardness and macroscopic mechanical properties in DP980 steels, Mater. Sci. Eng. A 597 (2014) 431–439, https://doi. org/10.1016/j.msea.2013.12.084. [35] K. Hasegawa, K. Kawamura, T. Urabe, Y. Hosoya, Effects of microstructure on stretch-flange-formability of 980 MPa grade cold-rolled ultra high strength steel sheets, ISIJ Int. 44 (2004) 603–609, https://doi.org/10.2355/ isijinternational.44.603. [36] J.H. Kim, M.G. Lee, D. Kim, D.K. Matlock, R.H. Wagoner, Hole-expansion formability of dual-phase steels using representative volume element approach with boundary-smoothing technique, Mater. Sci. Eng. A 527 (2010) 7353–7363, https://doi.org/10.1016/j.msea.2010.07.099. 11
0
Puede agregar este documento a su colección de estudio (s)
Iniciar sesión Disponible sólo para usuarios autorizadosPuede agregar este documento a su lista guardada
Iniciar sesión Disponible sólo para usuarios autorizados(Para quejas, use otra forma )